logo
Wuhan Fengfan International Trade Co.,Ltd. 86-27-85615818 info@fengfan.net
Rack Nickel Plating Additive Good Filling Performance Good Dispersing Ability

Rack Nickel Plating Additive Good Filling Performance Good Dispersing Ability

  • प्रमुखता देना

    Rack Nickel Plating Additive

    ,

    Good Filling Nickel Plating Additive

    ,

    Good Dispersing chemical nickel plating

  • प्रकार
    निकेल चढ़ाना
  • उपयोग
    रैक निकल चढ़ाना योजक
  • उपस्थिति
    रंगहीन तरल
  • उत्पत्ति के प्लेस
    चीन
  • ब्रांड नाम
    FENG FAN
  • मॉडल संख्या
    निकेल मैक्स 870
  • न्यूनतम आदेश मात्रा
    बातचीत योग्य
  • मूल्य
    विनिमय योग्य
  • पैकेजिंग विवरण
    मानक निर्यात पैकेजिंग
  • प्रसव के समय
    15-25 कार्य दिवस
  • भुगतान शर्तें
    एल/सी, डी/ए, डी/पी, टी/टी, वेस्टर्न यूनियन, मनीग्राम
  • आपूर्ति की क्षमता
    200000pcs/दिन

Rack Nickel Plating Additive Good Filling Performance Good Dispersing Ability

Nickel MAX 870 Rack Nickel Plating Additive

 

1) Operating Instruction

 

Formula and Operation Condition Range
Nickel Sulfate (NiSO4·7H2O) 180~250g/L
Nickel Chloride (NiCl2·6H2O) 45~55g/L
Boric Acid (H3BO3) 45~55g/L
Nickel MAX 870A brightener 0.2~0.4ml/L
Nickel MAX 870B softener 6~10ml/L
Y1 wetting agent 1~2ml/L
PH 3.8~4.5
Temperature 50~65℃
Cathode Current Density 2.5~8.0A/dm2
Anodic Current Density 1.0~3.0A/dm2
Filtration Recycle filteration continuously
Agitation Cathode moving or air agitation

 

2) Bath Preparation

 

1. Fill the tank with about 70% water, heat to 70~80℃.

 

2. Add boric acid (H3BO3), stir until it is thoroughly dissolved.

 

2. Add the measured nickel sulfate (NiSO4·7H2O) and nickel chloride (NiCl2·6H2O), and stir till they are thoroughly dissolved. Then add water to the volume.

 

4. Add 1-2 ml/L H2O2 (30%) after dilution, and stir for 2 hours.

 

5. Add nickel carbonate or 4% sodium hydroxide solution, and adjust pH to 5.2.

 

6. Then add 3~5 g/L activated carbon powder and stir the bath, and then filter after standing about 3 to 5 hours.

 

7. Add diluted sulfuric acid (5-10%) to adjust pH to around 4.

 

8. Use wavy metal plate as cathode, electrolyte until low current region turn black into light gray with small current density 0.1-0.4A/dm².

 

9. add Nickel MAX 870 additives, and then put into production.